SK Minerals & Additives Ltd. Discuss your requirementEnquire

ATH vs MDH vs APP for wire and cable compounds

· SK Minerals & Additives Ltd.

In short

ATH (aluminium hydroxide) and MDH (magnesium hydroxide) are mineral hydroxides that work by absorbing heat and releasing water, and they need high loadings. ATH suits lower processing temperatures, MDH higher ones. APP (ammonium polyphosphate) is a phosphorus-based additive that works by forming a char and is used at lower loadings, typically inside an intumescent system in polyolefins.

Comparison

The ATH and MDH columns, and the typical ranges, are general background: check them against your supplier's data sheet. Figures for HOFNIL grades are from our own data sheets.

PropertyATH (aluminium hydroxide)MDH (magnesium hydroxide)APP (ammonium polyphosphate)
How it worksDecomposes, absorbing heat and releasing waterDecomposes, absorbing heat and releasing waterAcid source in an intumescent system; forms an insulating char
Decomposition onsetTypically about 180-220 °CTypically about 300-340 °CHOFNIL-FR A2: 285 °C minimum; other grades vary
Typical loading in a polyolefin, by weightTypically 50-65%Typically 50-65%Typically lower, as part of a phosphorus-nitrogen system
Water released, share of additive massAbout 35%About 31%None (not a hydrate)
Processing limitThe low onset is a problem in polymers processed hotHigher; suits hotter extrusionDepends on the grade and coating
Effect on mechanical propertiesHigh loading reduces elongation and flexibilityThe same, unless surface-treatedLower loading, smaller effect
Halogen contentNoneNoneNone
SmokeTypically lowTypically lowDepends on the whole system
Solubility in waterVery lowVery lowHOFNIL-FR A2 and FR A2M: 0.50 g per 100 ml maximum at 25 °C

When to choose which

  • ATH: the compound is processed at low temperature (typically below about 200 °C), a high filler loading is acceptable and low smoke is the priority. Common in halogen-free cable compounds.
  • MDH: the polymer has to be processed hotter than ATH tolerates.
  • APP-based system: you need to cut the loading and protect flexibility or mechanical properties, in a polyolefin where intumescence suits. The system also needs a carbon source and a gas source, for example a melamine compound, and the result depends on the whole formulation.
  • Blends: many compounds combine a hydroxide with a phosphorus system to reduce the total loading. This needs trials.

Cable standards set the real targets: for example IEC 60754 for halogen acid gas, EN 50575 for reaction to fire, and RoHS and REACH for substances. Specify against the standard your customer names, and test your own compound.

Which of our products fits

Our flame retardants are on the phosphorus side of this comparison.

  • HOFNIL-FR A2 and FR A2M, ammonium polyphosphate. FR A2 is ammonium polyphosphate II. FR A2M is ammonium polyphosphate with a melamine coating, which improves thermal stability and water resistance. Data sheet values: FR A2 nitrogen 19.0-21.0%, phosphorus 20.0-22.0%, average particle size about 15 µm; FR A2M nitrogen 15.0-17.0%, phosphorus 31.0-32.0%, average particle size about 10-12 µm.
  • Flame retardants for polyethylene. HOFNIL-312A and FR A2M, for polyethylene cable insulation and sheathing. They work by intumescence, which reduces dark smoke and carbon monoxide during combustion. Loading of HOFNIL-312A in PE: 25-28% for UL 94 V-0.
  • HOFNIL-87R. A halogen-free phosphorus-nitrogen synergist. In wire and cable it helps reach the required LOI.

Products in this guide

Questions engineers and buyers ask

Why do ATH and MDH need such high loadings?

They act mainly by absorbing heat and releasing water, so the effect grows with the amount present. Typically 50-65% by weight is needed, which is why mechanical properties and processing suffer. This is general background.

Can I use ATH in polypropylene?

Polypropylene is generally processed close to or above the temperature at which ATH starts to decompose, so MDH or a phosphorus-based system is more usual. Confirm with trials on your own extrusion line.

Is APP a drop-in replacement for ATH?

No. The mechanism, loading and formulation differ. APP normally works inside a system with a carbon source and a gas source, so the formulation has to be redesigned and retested.

Does halogen-free mean low smoke?

Not automatically. Smoke depends on the polymer and the whole formulation. Mineral hydroxides are generally low-smoke; test your own compound.

Can I get samples and a price?

Yes. We quote on request and do not publish a price list. Tell us the polymer, the cable standard you work to and the quantity, and we will send the data sheet, a sample and a quote.

Related reading

Tell us what you're making.

Working on a compound this guide touches? Ask for a technical data sheet, a sample or a quote.

Discuss your requirement

Tell us what you're making.

Ask for a technical data sheet, a sample or a quote. We reply to the email address you give here.